Li-ion Battery Electrode/Li Chips

How to make water-based electrode (graphite for anode) for your reference :
 
1.  Weight Ratio
1.  (All other weights depends on how much active power  your will use) :
○   Active Powder  :  92.5 %
○   CMC  :  1.5 %
○   SBR liquid  :  2.5 %
○   Conductive  :  3.5 %
○   Absolute Alcohol  :  15 ml/kg graphite
○   De-Ionized water  :  At least 125 % of graphite
2.  Make liquid thickening agent  :  heat up de-ionized water to 60C and then slowly put the CMC into the water and keep stiring until all of it is dissolved.
Click picture below to view the video how to coat the electrode and then make a coin cell : 
3.  Add alcohol into 125 % de-ionized water and then add conductive powder and stir.
4.  Put active powder into 3 and stir*
5.  Add SBR into 4 and stir*
6.  Take a little sample and test the viscosity, it is OK to coat if the viscosity is between 3000 - 5000 mpa.s.    If the viscosity is over this range, add more de-ionized water;   if the viscosity is lower, add more binder  (CMC and SBR)
 